Metallurgy for the Junior Engineer Papers: Crystal Structure, the Iron-Carbon Diagram, Heat Treatment, Extraction and Corrosion

Metallurgy asks two questions: how is a metal got out of its ore, and how do its structure and treatment decide its properties? The Chemical and Metallurgical Assistant and Junior Engineer (mechanical) papers test the first-diploma answers. This chapter teaches the standing core: crystal structures and mechanical tests, the iron-carbon diagram and its heat treatments, blast-furnace and steel-making chemistry, and the corrosion and testing that keep structures safe. It is written from standing subject matter, not a notice.
Overview

1. Crystal structure, defects and mechanical tests

1 min read

Metals are crystalline: atoms sit on a repeating lattice. The common metallic lattices are body-centred cubic (BCC), face-centred cubic (FCC) and hexagonal close-packed (HCP). FCC and HCP are close-packed with an atomic packing factor of about 0.74 and a coordination number of 12; BCC packs 0.68 with 8 neighbours. Ductile metals such as copper, aluminium and austenitic steel are FCC because FCC has many slip systems; alpha iron and chromium are BCC; zinc and magnesium are HCP.

LatticeAtoms per cellCoordinationPacking factor
Simple cubic160.52
BCC280.68
FCC4120.74
HCP6120.74
  • Tensile test: the stress-strain curve gives yield strength, ultimate tensile strength, elongation (ductility) and, from the slope, Young's modulus.
  • Hardness: Brinell uses a hard ball, Vickers a diamond pyramid, Rockwell a diamond cone or small ball with a depth reading. Impact tests (Charpy, Izod) measure toughness.
  • Defects: vacancies (point), dislocations (line) and grain boundaries (surface). Dislocations make metals far weaker than a perfect crystal, and anything that blocks them (work hardening, alloying, fine grains) strengthens the metal.

Metals are crystalline: atoms sit on a repeating lattice. The common metallic lattices are body-centred cubic (BCC), face-centred cubic (FCC) and hexagonal close-packed (HCP). FCC and HCP…

2. The iron-carbon diagram and heat treatment

1 min read · 1 part

The diagram maps the phases of iron-carbon alloys. Ferrite (BCC) dissolves at most about 0.02% carbon; austenite (FCC) dissolves up to about 2.14%; cementite (Fe₃C) holds 6.67% carbon. The eutectoid point is near 0.76% carbon at 727 °C, where austenite turns into pearlite, a lamellar mixture of ferrite and cementite; the eutectic point is at 4.3% carbon and about 1,147 °C. Steels have under 2.14% carbon and cast irons above it.

The lever rule gives phase fractions. A 0.4% carbon steel just below 727 °C is ferrite plus pearlite; the pearlite fraction is (0.4 − 0.02) ÷ (0.76 − 0.02) = 0.51, so about 51% pearlite. Annealing (slow furnace cooling) softens; normalising (air cooling) refines grain; hardening (quenching from the austenite range) makes hard, brittle martensite; tempering (reheating below 727 °C) trades some hardness for toughness. Case hardening (carburising, nitriding) gives a hard skin on a tough core.

Cast ironCarbon formCharacter
WhiteCementiteVery hard, brittle
GreyGraphite flakesGood damping and machinability, weak in tension
MalleableGraphite nodules from heat-treated white ironTougher, some ductility
Spheroidal (SG)Graphite spheres (magnesium treated)Strong and ductile
⚠️ Martensite is not stable iron
Martensite forms only when cooling is fast enough to stop carbon leaving the lattice; it is a supersaturated, strained BCT structure, which is why it is hard and brittle and why a quenched part is always tempered.

The diagram maps the phases of iron-carbon alloys. Ferrite (BCC) dissolves at most about 0.02% carbon; austenite (FCC) dissolves up to about 2.14%; cementite (Fe₃C) holds 6.67% carbon. The…

3. Extraction, the blast furnace and steel-making

1 min read

Extraction runs in stages: ore dressing (crushing, magnetic separation, froth flotation for sulphides), reduction to metal and refining. In the blast furnace the charge of iron ore, coke and limestone is fed from the top and hot air is blown in at the bottom. Coke burns to give heat and carbon monoxide, which reduces the ore, Fe₂O₃ + 3CO → 2Fe + 3CO₂. Limestone decomposes and its lime joins the silica gangue as a fusible slag, CaO + SiO₂ → CaSiO₃, which floats on the molten pig iron. Reducing pure Fe₂O₃ gives 2 × 55.85 ÷ 159.7 of its mass as iron, about 700 kg per tonne.

  • Steel-making removes carbon, silicon, manganese, phosphorus and sulphur from pig iron by oxidation. The basic oxygen (LD) converter blows oxygen onto the molten metal; the electric arc furnace melts scrap.
  • Aluminium is made by electrolysing alumina dissolved in molten cryolite (the Hall-Héroult process), because it is too reactive to be reduced by carbon at ordinary furnace temperatures.
  • Copper from sulphide ore is concentrated by froth flotation, roasted and smelted to matte, converted to blister copper and refined electrolytically.

Extraction runs in stages: ore dressing (crushing, magnetic separation, froth flotation for sulphides), reduction to metal and refining. In the blast furnace the charge of iron ore, coke…

4. Casting, welding, corrosion and testing

1 min read · 2 parts

A casting shrinks as it solidifies, so a riser feeds liquid metal to the last part to freeze and a good design makes the thickest section solidify last. In welding, the metal beside the weld is reheated and forms a heat-affected zone whose grain and hardness change; high carbon content raises the risk of cracking, so such steels are preheated. Powder metallurgy presses and sinters powders to make porous bearings and hard tool materials.

Corrosion is an electrochemical cell: an anode where metal dissolves, a cathode where oxygen is reduced and an electrolyte. Protection works by cutting off the electrolyte (paint, plating), by making the structure the cathode (cathodic protection, using a sacrificial zinc or magnesium anode, as in galvanising) or by alloying (stainless steel forms a chromium-oxide film). Non-destructive testing finds flaws without damage: dye penetrant for surface cracks in any non-porous metal, magnetic particle for surface and near-surface flaws in ferromagnetic metal only, ultrasonic for internal flaws and radiography for internal voids.

🎯 Zinc protects even when scratched
Zinc is more reactive than iron, so on a galvanised sheet with a scratch the zinc corrodes in preference and the exposed iron stays cathodic. Tin, being less reactive than iron, protects only while the coating is intact.

A casting shrinks as it solidifies, so a riser feeds liquid metal to the last part to freeze and a good design makes the thickest section solidify last. In welding, the metal beside the…

5. Worked problems: the lever rule and Brinell hardness

1 min read · 1 part

The lever rule turns the iron-carbon diagram into numbers. Below 727 °C a slow-cooled steel with less than 0.76% carbon is a mixture of proeutectoid ferrite and pearlite. For a 0.40% carbon steel, with ferrite holding 0.02% C and pearlite 0.76% C, the fraction of pearlite is (0.40 − 0.02) ÷ (0.76 − 0.02) = 0.38 ÷ 0.74 = 51%, and the rest, 49%, is ferrite. The arm of the lever opposite a phase gives that phase, so the pearlite fraction is measured from the ferrite end. Dropping the 0.02% ferrite solubility gives 0.40 ÷ 0.76 = 53%, a small but examinable difference.

TreatmentCoolingResult
AnnealingSlow, in the furnaceSoft, ductile, stress-relieved
NormalisingIn still airFiner grains, somewhat harder than annealed
HardeningQuenching in water or oilMartensite: very hard and brittle
TemperingReheating the quenched steel below 727 °CLess brittle, with some hardness given up

Brinell hardness is the load divided by the curved area of the impression: HB = 2P ÷ [πD (D − √(D² − d²))]. For a 10 mm ball under 3,000 kgf that leaves a 4 mm impression, √(100 − 16) = 9.165, so HB = 6,000 ÷ [π × 10 × 0.835] = 229.

ℹ️ Which hardness test for which job
Brinell uses a large ball and suits soft metals and castings; Rockwell reads the depth of a small indentation directly and is quick for hardened steel; Vickers uses a diamond pyramid and covers the whole range, including thin sections.

The lever rule turns the iron-carbon diagram into numbers. Below 727 °C a slow-cooled steel with less than 0.76% carbon is a mixture of proeutectoid ferrite and pearlite. For a 0.40% carbon…

Second Pass: Unit-cell Counts, Cooling Rates, Special Points and Ore Richness

1 min read · 2 parts

A cubic unit cell holds 2 atoms in BCC and 4 in FCC; the packing factors are 0.68 for BCC, 0.74 for FCC and HCP. The eutectoid point of steel is 0.76% C at 727 °C and the eutectic of cast iron is 4.3% C at 1147 °C. Cooling rate rises from annealing (furnace) through normalising (air) to quenching (water).

Worked values
ItemWorkingAnswer
Atoms per FCC unit cell8 × 1/8 + 6 × 1/24
Fe in Fe₃O₄ (Fe = 55.85, O = 16)167.55/231.5572.4%
Eutectic of cast iron—4.3% C, 1147 °C
Eutectoid steel—0.76% C, all pearlite
ℹ️ Cooling rate decides the structure
Furnace cooling (annealing) gives coarse pearlite and the softest steel, air cooling (normalising) gives finer pearlite and more strength, and quenching in water traps carbon in hard, brittle martensite, which tempering then toughens.

A cubic unit cell holds 2 atoms in BCC and 4 in FCC; the packing factors are 0.68 for BCC, 0.74 for FCC and HCP. The eutectoid point of steel is 0.76% C at 727 °C and the eutectic of cast…

Key takeaways

  • FCC and HCP pack 74% with 12 neighbours, BCC 68% with 8; FCC metals are the ductile ones.
  • Ferrite holds 0.02% C, austenite 2.14%, cementite 6.67%; eutectoid 0.76% C at 727 °C gives pearlite; the lever rule gives the fractions.
  • Quench to martensite, then temper; annealing softens and normalising refines grain.
  • The blast furnace reduces ore with CO and limestone makes slag; aluminium needs electrolysis in cryolite.
  • Corrosion is an electrochemical cell; sacrificial anodes and passive films protect, and magnetic-particle testing needs a ferromagnetic metal.
  • Lever rule for a hypo-eutectoid steel: pearlite = (C − 0.02) ÷ (0.76 − 0.02); Brinell HB = 2P ÷ [πD (D − √(D² − d²))].

Practice questions (25)

Attempt each one before opening the answer. Every explanation names the tempting wrong option as well as the right one, because that is where marks are lost.

  1. The atomic packing factor of a face-centred cubic lattice is about:

    1. 0.52
    2. 0.68
    3. 0.74
    4. 0.91
    Show answer

    Answer: C — 0.74

    FCC (and HCP) are close-packed with a packing factor of π√2 ÷ 6 ≈ 0.74. Simple cubic is 0.52 and BCC is 0.68, so 0.74 is the highest possible for equal spheres.
  2. The maximum solubility of carbon in austenite is about:

    1. 0.02%
    2. 0.76%
    3. 2.14%
    4. 6.67%
    Show answer

    Answer: C — 2.14%

    Austenite, being FCC with larger interstitial gaps, dissolves up to about 2.14% carbon at 1,147 °C. Ferrite holds only about 0.02%, 0.76% is the eutectoid composition and 6.67% is the carbon content of cementite.
  3. A plain carbon steel with 0.4% carbon is slowly cooled to just below 727 °C. Taking the ferrite limit as 0.02% and the eutectoid composition as 0.76%, the fraction of pearlite is about:

    1. 49%
    2. 51%
    3. 40%
    4. 95%
    Show answer

    Answer: B — 51%

    By the lever rule the pearlite fraction is (0.4 − 0.02) ÷ (0.76 − 0.02) = 0.38 ÷ 0.74 = 0.51. The 49% figure is the ferrite share, and 40% simply repeats the carbon content.
Show the other 22 questions
  1. Tempering is carried out on a quenched steel mainly to:

    1. reduce brittleness and internal stress at some cost in hardness
    2. increase the carbon content
    3. convert it fully back to austenite
    4. make it magnetic
    Show answer

    Answer: A — reduce brittleness and internal stress at some cost in hardness

    Quenched martensite is hard but brittle and full of stress. Reheating below 727 °C lets some carbon precipitate as fine carbide, relieving stress and restoring toughness while keeping much of the hardness.
  2. In the blast furnace, limestone is added mainly to:

    1. combine with silica impurities to form a fusible slag
    2. supply carbon monoxide
    3. raise the melting point of the charge
    4. absorb oxygen from the blast
    Show answer

    Answer: A — combine with silica impurities to form a fusible slag

    Limestone decomposes to lime, which combines with silica in the gangue to form calcium silicate slag. The slag melts, floats on the pig iron and is tapped off separately; carbon monoxide comes from the coke.
  3. Taking Fe = 55.85 and O = 16, the mass of iron obtained by completely reducing 1,000 kg of pure Fe₂O₃ is about:

    1. 700 kg
    2. 300 kg
    3. 1,000 kg
    4. 350 kg
    Show answer

    Answer: A — 700 kg

    Fe₂O₃ has molar mass 159.7 and holds 111.7 of iron, so 1,000 × 111.7 ÷ 159.7 ≈ 700 kg. The 300 kg figure is the oxygen share, which is lost as CO₂ in the furnace.
  4. A galvanised iron sheet is scratched through to the iron. The iron still resists rusting because:

    1. zinc, being more reactive, corrodes in preference and acts as a sacrificial anode
    2. zinc is less reactive than iron
    3. zinc is a good insulator of electricity
    4. iron cannot corrode in a dry atmosphere
    Show answer

    Answer: A — zinc, being more reactive, corrodes in preference and acts as a sacrificial anode

    Zinc lies above iron in the reactivity series, so in the corrosion cell zinc is the anode and dissolves while iron is the cathode. This sacrificial protection continues until the nearby zinc is used up.
  5. Which non-destructive test can be used only on ferromagnetic materials?

    1. Magnetic particle inspection
    2. Dye penetrant inspection
    3. Ultrasonic testing
    4. Radiography
    Show answer

    Answer: A — Magnetic particle inspection

    Magnetic particle inspection magnetises the part and iron powder gathers where a flaw leaks flux, which needs a material that can be magnetised. Dye penetrant, ultrasonic and radiographic methods work on non-magnetic metals too.
  6. A slow-cooled 0.40% carbon steel has ferrite at 0.02% C and pearlite at 0.76% C just below 727 °C. The fraction of pearlite is nearest to:

    1. 51%
    2. 53%
    3. 40%
    4. 74%
    Show answer

    Answer: A — 51%

    Lever rule: (0.40 − 0.02) ÷ (0.76 − 0.02) = 0.38 ÷ 0.74 = 51%. Ignoring the ferrite solubility gives 0.40 ÷ 0.76 = 53%, the near-miss option.
  7. A 10 mm ball under a load of 3,000 kgf leaves an impression of diameter 4 mm. The Brinell hardness number is nearest to:

    1. 229
    2. 458
    3. 115
    4. 300
    Show answer

    Answer: A — 229

    HB = 2P ÷ [πD (D − √(D² − d²))] = 6,000 ÷ [π × 10 × (10 − 9.165)] = 6,000 ÷ 26.2 = 229. Forgetting the factor 2 in the numerator halves the answer to about 115.
  8. The number of atoms effectively belonging to one face-centred cubic unit cell is:

    1. 4
    2. 2
    3. 6
    4. 14
    Show answer

    Answer: A — 4

    Eight corner atoms contribute 1/8 each and six face atoms 1/2 each: 1 + 3 = 4. A BCC cell has 2 atoms.
  9. The carbon content and temperature of the eutectic point in the iron–carbon diagram are about:

    1. 4.3% C and 1147 °C
    2. 0.76% C and 727 °C
    3. 2.1% C and 1493 °C
    4. 6.67% C and 1538 °C
    Show answer

    Answer: A — 4.3% C and 1147 °C

    The eutectic (liquid to austenite plus cementite) lies at 4.3% C and 1147 °C, which is why cast irons melt at lower temperatures than steels. 0.76% and 727 °C is the eutectoid.
  10. Arrange the heat treatments of steel in increasing order of cooling rate:

    1. Annealing, normalising, quenching
    2. Quenching, normalising, annealing
    3. Normalising, annealing, quenching
    4. Annealing, quenching, normalising
    Show answer

    Answer: A — Annealing, normalising, quenching

    Annealing cools slowly in the furnace, normalising cools in still air and quenching cools rapidly in water or oil, so the cooling rate rises in that order.
  11. The iron content by mass of the ore magnetite, Fe₃O₄ (Fe = 55.85, O = 16), is nearest to:

    1. 72%
    2. 70%
    3. 77%
    4. 64%
    Show answer

    Answer: A — 72%

    Fe = 3 × 55.85 = 167.55 and Fe₃O₄ = 167.55 + 64 = 231.55, so Fe = 72.4%. Haematite Fe₂O₃ has 69.9%.
  12. A steel with exactly 0.76% carbon cooled slowly below 727 °C consists of:

    1. 100% pearlite
    2. Ferrite and pearlite
    3. Pearlite and cementite
    4. Martensite
    Show answer

    Answer: A — 100% pearlite

    At the eutectoid composition austenite transforms wholly to pearlite, a lamellar mixture of ferrite and cementite. Hypoeutectoid steels add proeutectoid ferrite and hypereutectoid steels proeutectoid cementite.
  13. The hardness test that uses a diamond pyramid indenter with an included angle of 136° is the:

    1. Vickers test
    2. Brinell test
    3. Rockwell C test
    4. Charpy test
    Show answer

    Answer: A — Vickers test

    The Vickers test presses a square-based diamond pyramid (136° between faces). Brinell uses a hard steel ball, Rockwell C a diamond cone and Charpy measures impact energy, not hardness.
  14. The number of atoms effectively contained in a body-centred cubic (BCC) unit cell is:

    1. 4
    2. 1
    3. 6
    4. 2
    Show answer

    Answer: D — 2

    BCC has 8 corner atoms each shared by 8 cells (1) plus 1 at the centre, so 2 atoms. Four is the FCC count, the tempting neighbour.
  15. Consider the following statements:
    1. FCC and HCP (ideal) structures both have an atomic packing factor of about 0.74.
    2. The coordination number is 12 in both FCC and HCP.
    Which of the statements given above is/are correct?

    1. Both 1 and 2
    2. 1 only
    3. 2 only
    4. Neither 1 nor 2
    Show answer

    Answer: A — Both 1 and 2

    Both are close-packed structures with packing factor 0.74 and coordination number 12. BCC has 0.68 and 8, the tempting lower values.
  16. A slow-cooled 0.6% carbon steel just below 727 °C has ferrite (0.02% C) and pearlite (0.76% C). The fraction of pearlite is about:

    1. 76%
    2. 60%
    3. 22%
    4. 78%
    Show answer

    Answer: D — 78%

    Lever rule: pearlite = (0.60 − 0.02) ÷ (0.76 − 0.02) = 0.58 ÷ 0.74 = 78%. The 22% is the ferrite fraction, the tempting complement.
  17. Cementite (Fe₃C) contains about what percentage of carbon by mass?

    1. 6.67%
    2. 4.3%
    3. 0.76%
    4. 2.14%
    Show answer

    Answer: A — 6.67%

    Cementite is the iron carbide with 6.67% carbon. 0.76% is the eutectoid composition and 4.3% the eutectic, both tempting figures from the same diagram.
  18. Case hardening by carburising is a process in which:

    1. Carbon is diffused into the surface of low-carbon steel to harden the skin and keep a tough core
    2. The steel is cooled to a very low temperature
    3. The whole steel is heated and cooled slowly
    4. Zinc is coated on the surface
    Show answer

    Answer: A — Carbon is diffused into the surface of low-carbon steel to harden the skin and keep a tough core

    Carburising adds carbon to the surface layer and the part is then quenched, giving a hard case over a tough core. Slow furnace cooling describes annealing, the tempting confusion.
  19. Aluminium is extracted industrially from alumina by:

    1. Roasting in air
    2. Reduction with carbon in a blast furnace
    3. Electrolysis in molten cryolite (Hall–Héroult process)
    4. Reduction with hydrogen gas
    Show answer

    Answer: C — Electrolysis in molten cryolite (Hall–Héroult process)

    Alumina dissolved in molten cryolite is electrolysed because aluminium is too reactive for carbon reduction, so the blast-furnace method is the tempting wrong option.
  20. Using Al = 27 and O = 16, the mass of aluminium obtained from 102 kg of pure Al₂O₃ is:

    1. 102 kg
    2. 27 kg
    3. 81 kg
    4. 54 kg
    Show answer

    Answer: D — 54 kg

    Molar mass of Al₂O₃ = 2 × 27 + 3 × 16 = 102, so 102 kg is one kilomole giving 2 kmol Al = 54 kg. The 27 kg is the mass of one kmol only.
  21. The sacrificial anode used to protect a steel pipeline from corrosion is made of a metal that is:

    1. Less reactive than iron, such as copper
    2. More reactive (more anodic) than iron, such as zinc or magnesium
    3. A non-metal
    4. Identical to the pipe steel
    Show answer

    Answer: B — More reactive (more anodic) than iron, such as zinc or magnesium

    The more anodic metal corrodes in preference and protects the steel, which is why zinc and magnesium are used. A less reactive metal such as copper would make the steel corrode faster, the tempting error.
  22. Assertion (A): Quenched plain carbon steel is hard but brittle.
    Reason (R): Rapid cooling traps carbon in a distorted lattice, forming martensite.
    Which one of the following is correct?

    1. Both A and R are true, and R is the correct explanation of A
    2. Both A and R are true, but R is not the correct explanation of A
    3. A is true, but R is false
    4. A is false, but R is true
    Show answer

    Answer: A — Both A and R are true, and R is the correct explanation of A

    Martensite is a supersaturated, strained structure, which gives hardness and brittleness, so R explains A. Tempering is the follow-up that restores toughness, a point that is not part of this reason.