Joining, Powder and Polymer Processing in Numbers: Arc Heat Input and Cooling Rate, Resistance and Friction Welding, Brazing, Sintering, Injection Moulding, Extrusion and Composites

Section 3 of the PI paper names 'heat transfer and associated losses' in fusion welding, solid-state and resistance processes, compaction and sintering, and polymer and composite moulding, and the chapters before this one give them no numbers. An arc at 24 V and 200 A travelling at 5 mm/s delivers 960 J/mm and, at 80% efficiency, 768 J/mm to the plate, which cools a thick plate at about 63 K/s through 550 °C. A spot weld of 10 kA for 0.2 s through 100 µΩ develops 2 kJ, of which only about 43% melts the nugget. A sintered iron compact moving from density 6.3 to 7.0 g/cm³ shrinks 3.5% linearly; a 150 cm² moulding at 40 MPa needs 600 kN of clamp; and a 60% carbon–epoxy ply has a fibre-direction modulus of 139 GPa.
Overview

Fusion Welding: Heat Input, Cooling Rate, Melting Efficiency and Losses

2 min read · 1 part

Fusion welding melts the joint with a concentrated heat source, and the quantity that governs the metallurgy is the heat input per unit length: H = η V I / v. Here V = 24 V, I = 200 A, travel speed v = 5 mm/s: the gross figure is VI/v = 960 J/mm. The arc efficiency η is the fraction that enters the work: about 0.8 for SMAW, GMAW and SAW (the slag blanket of SAW traps the heat and reaches 0.9+), 0.6–0.7 for GTAW, and 0.2–0.5 for laser and electron beam depending on reflectivity. The losses are radiation, convection, spatter and, for laser, reflection. At η = 0.8 the net input is 768 J/mm. For a thick plate (three-dimensional heat flow, Rosenthal) the cooling rate at temperature T is dT/dt = 2πk (T − T₀)²/H_net; with k = 0.028 W/mm·K, T = 550 °C and T₀ = 25 °C this is 63 K/s. Halving the heat input doubles the rate, which is why low-heat-input welds and cold plates harden the heat-affected zone of steel; preheating cuts the rate (the T₀ term) and slows cracking. A thin plate behaves differently: dT/dt = 2πkρc(h/H_net)²(T − T₀)³, so the rate falls as the square of the heat input.

Melting efficiency f₂ is the share of the net input that actually melts metal rather than heating the plate. The energy to melt steel from room temperature, including latent heat, is about 10.3 J/mm³, so a fusion zone of area A needs H_net f₂ = A × 10.3: with f₂ = 0.5 the cross-section melted is 37 mm² (about a 10 mm × 3.7 mm section) and the volume rate is A v = 186 mm³/s. Notice the two efficiencies: arc efficiency (source to plate) and melting efficiency (plate to molten metal); their product, 0.4 here, is the fraction of electrical power that becomes weld metal. SAW and electroslag have the highest, because the heat is confined; GTAW the lowest, but it gives the best control at 1–3 mm.

ProcessArc efficiency ηNote
SAW0.9–1.0Heat trapped under flux
SMAW, GMAW0.7–0.85Spatter and radiation losses
GTAW0.6–0.7Best control, thin sections
Laser, electron beam0.2–0.5Reflectivity; keyhole raises it

Fusion welding melts the joint with a concentrated heat source, and the quantity that governs the metallurgy is the heat input per unit length: H = η V I / v. Here V = 24 V, I = 200 A…

Resistance and Solid-State Welding, Brazing and Adhesives

2 min read · 2 parts

Resistance welding generates heat by Joule's law Q = I² R t. For 10 kA, a total circuit resistance of 100 µΩ and 0.2 s: Q = 2000 J. A nugget 6 mm in diameter through 3 mm of steel has a volume of 0.0 mm³ and needs 860 J to melt (1.3 MJ/kg with latent heat), i.e. only 43% of the energy; the rest conducts into the electrodes (water-cooled copper) and the sheet. Current, time and force are the three variables; too short a time with too high a current expels metal. Friction welding of two 20 mm rods at 1500 rpm under 30 MPa has an axial force of 9.4 kN and, with μ = 0.4, a heating power of (2/3)πμpωR³ = 3.9 kW; flash and upset follow. Friction-stir welding heats by a rotating non-consumable tool (shoulder radius 7.5 mm, 1000 rpm, 40 MPa): about 1480 W, and it stays below melting, which avoids porosity and solidification cracking in aluminium. Ultrasonic welding joins thin foils at about 20 kHz by interfacial scrubbing, without heat input from outside.

Brazing and soldering join without melting the parent metal; the filler (above 450 °C for brazing, below for soldering) is drawn into the gap by capillary action, which is why the gap is 0.05–0.25 mm: for two parallel plates a gap g = 0.1 mm, surface tension 0.9 N/m, contact angle 10° and density 8000 kg/m³ give a rise 2γ cosθ/(ρ g_grav g) = 226 mm, far more than needed. Adhesive joints carry shear, so a single-lap joint of 25 mm × 12.5 mm with τ = 18 MPa carries 5625 N; peel and cleavage loads are weak and must be designed out, and surface preparation matters more than adhesive strength.

ProcessHeat sourceKey relation
Resistance spotJoule heating at interfaceQ = I² R t
Friction weldingRubbing of rotating rod(2/3) π μ p ω R³
Friction stirRotating tool, solid stateBelow melting point
BrazingFiller melts, parent does notCapillary gap 0.05–0.25 mm

Resistance welding generates heat by Joule's law Q = I² R t. For 10 kA, a total circuit resistance of 100 µΩ and 0.2 s: Q = 2000 J. A nugget 6 mm in diameter through 3 mm of steel has a…

Powder Metallurgy: Density, Compaction and Sintering

1 min read

Powders are made by atomisation, reduction of oxides, electrolysis or milling, then compacted in a die at 200–800 MPa and sintered at 70–90% of the melting temperature in a protective atmosphere. The compaction force is pressure times the area: 600 MPa on a 20 mm diameter punch is 188 kN, which sets the press size. Density tracks the process: iron has a theoretical density of 7.87 g/cm³; a green compact at 6.3 g/cm³ has porosity 1 − 6.3/7.87 = 19.9%, a sintered part at 7.0 g/cm³ has 11.1%, and since the mass is unchanged the part shrinks linearly by 1 − (ρ_g/ρ_s)^(1/3) = 3.45%. The fill ratio (apparent density 2.6 g/cm³ to green 6.3) is 2.4, so the die cavity is 2.4 times deeper than the finished part. Mixed powders use the inverse-mixture law: 90% Cu (8.96 g/cm³) and 10% Sn (7.31) by weight have a theoretical density of 8.76 g/cm³ — not the 8.80 an arithmetic mean by weight would claim. Design limits: low aspect ratio, no undercuts, uniform section, because the powder does not flow sideways and density falls with depth (friction at the die wall), which is why double-acting presses compact from both ends.

StateDensity (g/cm³)Porosity
Apparent (loose)2.667.0%
Green compact6.319.9%
Sintered7.011.1%

Powders are made by atomisation, reduction of oxides, electrolysis or milling, then compacted in a die at 200–800 MPa and sintered at 70–90% of the melting temperature in a protective…

Polymer Processing and Composites

2 min read · 3 parts

Injection moulding: the machine is sized by the clamping force F = projected area × cavity pressure: 150 cm² at 40 MPa needs 600 kN. The cycle is dominated by cooling, the conduction time for a slab of thickness h: t = h²/(π²α) ln[4(T_i − T_m)/(π(T_e − T_m))]; with h = 3 mm, α = 0.1 mm²/s, melt 220 °C, mould 40 °C and ejection at 80 °C: 15.9 s, and t scales as h², so halving the wall thickness cuts cooling four-fold — the reason for thin, ribbed walls. The extruder output in drag flow is Q = ½π²D²N h sin φ cos φ; for D = 60 mm, N = 1 rev/s, channel depth 3 mm and helix 17.66°: 15.4 cm³/s, less the pressure back-flow. In blow moulding the wall thins in proportion to the blow-up ratio: a 4 mm parison of 40 mm diameter blown into a 100 mm mould leaves a 1.6 mm wall (t_f = t_p D_p/D_m, a thin-wall approximation). Thermoforming thins the sheet where it stretches most (the cup bottom corner); compression moulding suits thermosets; calendering makes film and sheet by squeezing through hot rolls.

Composite moulding (hand lay-up, filament winding, pultrusion, autoclave) places fibre in a matrix, and the property follows the rule of mixtures. Along the fibres E_c = V_f E_f + (1 − V_f)E_m = 0.6 × 230 + 0.4 × 3.5 = 139.4 GPa for carbon in epoxy; across them the inverse rule gives E_t = 1/(V_f/E_f + (1 − V_f)/E_m) = 8.6 GPa, about 2% of the longitudinal value — hence the cross-plied laminate. Density mixes the same way: 0.6 × 1.8 + 0.4 × 1.2 = 1.56 g/cm³, which gives a specific stiffness many times steel's.

ProcessSizing relationValue here
Injection clamp forceA_proj × p_cav600 kN
Cooling timeh²/(π²α) ln(…)15.9 s
Fibre-direction modulusV_f E_f + (1 − V_f)E_m139.4 GPa
Transverse modulusinverse rule8.6 GPa
🎯 Resistance welding heat, computed
The heat generated at a resistance spot weld is H = I²Rt. For I = 10 kA, a contact resistance of 100 µΩ and 0.2 s, H = 10⁸ × 10⁻⁴ × 0.2 = 2000 J. Because heat goes as the square of the current, a 10% increase in current raises it by 21%, which is why current is the dominant variable and the weld nugget is very sensitive to it. Current, time and electrode force are the three parameters; too little force raises contact resistance and causes expulsion of molten metal.

Injection moulding: the machine is sized by the clamping force F = projected area × cavity pressure: 150 cm² at 40 MPa needs 600 kN. The cycle is dominated by cooling, the conduction time…

Key takeaways

  • Heat input per length is η V I / v; cooling rate in a thick plate is 2πk(T − T₀)²/H_net, so doubling the heat input halves it and preheating lowers it.
  • Resistance welding Q = I² R t converts only a small share of energy to nugget; friction-stir welding stays below melting.
  • In powder metallurgy porosity = 1 − ρ/ρ_theoretical, linear sintering shrinkage = 1 − (ρ_green/ρ_sintered)^(1/3), and mixed densities use the inverse rule by weight.
  • Injection clamp force is projected area × cavity pressure; cooling time scales as thickness squared.
  • Composite modulus: parallel (rule of mixtures) along fibres, inverse rule across fibres.

Practice questions (24)

Attempt each one before opening the answer. Every explanation names the tempting wrong option as well as the right one, because that is where marks are lost.

  1. An arc welding source of 24 V and 200 A travels at 5 mm/s with an arc efficiency of 0.8. The net heat input per unit length is:

    1. 4800 J/mm
    2. 768 J/mm
    3. 76.8 J/mm
    4. 960 J/mm
    Show answer

    Answer: B — 768 J/mm

    H = ηVI/v = 0.8 × 24 × 200/5 = 768 J/mm. The gross value 960 J/mm omits the efficiency; multiplying by the speed instead of dividing is the unit slip.
  2. If the heat input of a thick-plate arc weld is halved, the cooling rate through a given temperature:

    1. Increases by a factor of 2, since rate varies inversely with H_net
    2. Increases by a factor of 4
    3. Stays the same
    4. Halves
    Show answer

    Answer: A — Increases by a factor of 2, since rate varies inversely with H_net

    In the thick-plate (Rosenthal) solution dT/dt = 2πk(T − T₀)²/H_net: the rate is inversely proportional to the heat input, so halving H doubles the rate. The square is on the temperature difference — preheating a plate lowers the rate by a squared factor. (Thin plates differ: the rate goes as H⁻² there.)
  3. For the 24 V, 200 A, 5 mm/s weld at 80% efficiency on thick steel plate (k = 0.028 W/mm·K, T₀ = 25 °C), the cooling rate at 550 °C in K/s (nearest integer) is:

    Numerical answer — type the value.

    Show answer

    Answer: 63

    H_net = 768 J/mm; dT/dt = 2π × 0.028 × 525²/768 = 63.1 K/s. Using the gross 960 J/mm would give 51 K/s.
Show the other 21 questions
  1. A resistance spot weld passes 10 kA for 0.2 s through a total resistance of 100 µΩ. The heat generated in J is:

    Numerical answer — type the value.

    Show answer

    Answer: 2000

    Q = I²Rt = (10⁴)² × 100 × 10⁻⁶ × 0.2 = 2000 J. Forgetting to square the current is the usual error.
  2. Friction-stir welding is classed as a solid-state process because:

    1. It needs a filler wire
    2. It is done in a vacuum
    3. It uses no tool
    4. The metal is softened and stirred below its melting point
    Show answer

    Answer: D — The metal is softened and stirred below its melting point

    A rotating tool plasticises the metal by friction and stirs it across the joint without reaching the melting point, so there is no solidification cracking or porosity; no filler or shielding gas is needed, and it works in air.
  3. A green iron compact has density 6.3 g/cm³ and sinters to 7.0 g/cm³ with no mass loss. Its linear shrinkage in per cent (two decimals) is:

    Numerical answer — type the value.

    Show answer

    Answer: 3.45

    Mass is fixed, so volume scales as 1/ρ and length as ρ^(−1/3): shrinkage = 1 − (6.3/7.0)^(1/3) = 3.45%. The volumetric shrinkage is 10%, three times larger.
  4. Mixed 90% Cu (8.96 g/cm³) and 10% Sn (7.31 g/cm³) powders by weight have a theoretical density of about:

    1. 8.80 g/cm³ — the weighted mean of densities
    2. 8.14 g/cm³ — the simple average
    3. 9.50 g/cm³
    4. 8.76 g/cm³ — the inverse rule 1/ρ = Σw/ρ
    Show answer

    Answer: D — 8.76 g/cm³ — the inverse rule 1/ρ = Σw/ρ

    Mass fractions add volumes, not densities: 1/ρ = 0.9/8.96 + 0.1/7.31, giving 8.76. The arithmetic weighted mean 8.80 is close but wrong in principle; for large density differences it fails badly.
  5. An injection moulding of projected area 150 cm² has a cavity pressure of 40 MPa. The minimum clamp force in kN is:

    Numerical answer — type the value.

    Show answer

    Answer: 600

    F = pA = 40 × 10⁶ × 150 × 10⁻⁴ = 600000 N = 600 kN. The area is the projection on the parting plane, not the surface area of the part.
  6. Which statements about composites and polymer processing are correct?

    1. Compression moulding is the usual method for thermoplastic bottles
    2. The longitudinal modulus of a unidirectional ply follows the rule of mixtures
    3. The transverse modulus of a unidirectional ply follows the inverse rule and is far lower
    4. Injection-moulding cooling time varies as the square of wall thickness
    Show answer

    Answer: B — The longitudinal modulus of a unidirectional ply follows the rule of mixtures; C — The transverse modulus of a unidirectional ply follows the inverse rule and is far lower; D — Injection-moulding cooling time varies as the square of wall thickness

    Parallel loading adds stiffness by volume fraction and series loading adds compliance; conduction time goes as h². Bottles are blow moulded; compression moulding is mainly for thermosets.
  7. In arc welding, the heat input per unit length of weld is given by

    1. V/I
    2. η·V·I/v (voltage × current × efficiency ÷ travel speed)
    3. I/v
    4. V·I·v
    Show answer

    Answer: B — η·V·I/v (voltage × current × efficiency ÷ travel speed)

    Heat input H = ηVI/v, so slower travel or higher VI deposits more heat per length. Multiplying by v instead of dividing wrongly makes faster welding hotter, the tempting slip.
  8. Brazing differs from fusion welding in that brazing

    1. melts the base metals
    2. needs no filler
    3. joins without melting the base metals, using a filler above 450 °C
    4. uses filler below 450 °C
    Show answer

    Answer: C — joins without melting the base metals, using a filler above 450 °C

    Brazing melts only a filler (above 450 °C) that wets the unmelted base metals by capillarity. Melting the base metal is welding, and filler below 450 °C is soldering, the tempting neighbours.
  9. In powder metallurgy the "green compact" is

    1. the raw powder
    2. the pressed but not yet sintered powder part
    3. the fully sintered part
    4. a molten part
    Show answer

    Answer: B — the pressed but not yet sintered powder part

    The green compact is the pressed powder that has handling strength but has not been sintered. The fully bonded part comes only after sintering, the tempting later stage.
  10. In a fibre-reinforced polymer composite, the fibres primarily provide

    1. the colour
    2. the binding matrix
    3. strength and stiffness along their direction
    4. electrical insulation only
    Show answer

    Answer: C — strength and stiffness along their direction

    Strong, stiff fibres carry most of the load along their axis while the matrix transfers stress between them. The matrix, not the fibre, is the binder, the tempting role swap.
  11. An arc weld uses 25 V, 200 A, a travel speed of 5 mm/s and an efficiency of 0.9. The heat input, in J/mm, is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 900

    H = ηVI/v = 0.9 × 25 × 200/5 = 4500/5 = 900 J/mm. Forgetting the efficiency gives 1000 J/mm, overstating the heat actually delivered.
  12. For an arc at 25 V and 200 A, the electrical power drawn, in kW, is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 5

    P = VI = 25 × 200 = 5000 W = 5 kW. Adding V and I (225) is dimensionally meaningless for power. Substituting the answer back into the relation confirms it.
  13. Which of the following are solid-state (no melting of base metal) joining processes?

    1. Explosive welding
    2. Diffusion bonding
    3. Friction welding
    4. Gas metal arc welding
    Show answer

    Answer: A — Explosive welding; B — Diffusion bonding; C — Friction welding

    Friction, diffusion and explosive welding join without melting the base metal. GMAW is a fusion process that melts the base metal, so it is the exception.
  14. A sintered part has a density of 6.8 g/cm³ against a theoretical (pore-free) density of 8.0 g/cm³. Its relative density, as a fraction (two decimals), is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 0.85

    Relative density = 6.8/8.0 = 0.85, so porosity is 15%. Subtracting (8.0 − 6.8 = 1.2) gives the density deficit, not the relative density.
  15. A unidirectional composite has 60% fibre (E = 400 GPa) and 40% matrix (E = 3 GPa) by volume. Its longitudinal modulus by the rule of mixtures, in GPa (one decimal), is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 241.2

    E_c = V_f·E_f + V_m·E_m = 0.6 × 400 + 0.4 × 3 = 240 + 1.2 = 241.2 GPa. The transverse (inverse) rule gives a far lower value and does not apply along the fibres.
  16. Direct current electrode positive (DCEP, reverse polarity) in arc welding generally gives

    1. a faster electrode melting rate than penetration
    2. no arc at all
    3. deeper penetration into the workpiece
    4. cold joints always
    Show answer

    Answer: C — deeper penetration into the workpiece

    With the electrode positive, most heat is at the work, giving deep penetration. Electrode-negative (straight polarity) melts the electrode faster with shallower penetration, the tempting swap.
  17. Powder metallurgy is especially advantageous for making

    1. porous self-lubricating bearings and parts from refractory or immiscible metals
    2. one-off hand-forged tools
    3. parts that must be fully dense only
    4. large single castings
    Show answer

    Answer: A — porous self-lubricating bearings and parts from refractory or immiscible metals

    PM can build controlled porosity (oil-retaining bearings) and consolidate high-melting or immiscible metals hard to cast. Making only fully dense parts is not its special strength, since controlled porosity is a key PM advantage, the tempting limiter.
  18. In resistance spot welding, the heat generated is governed by

    1. H = I/Rt
    2. H = I²Rt (current squared × resistance × time)
    3. H = IRt
    4. H = V²t only
    Show answer

    Answer: B — H = I²Rt (current squared × resistance × time)

    Joule heating gives H = I²Rt, so current has the strongest effect (squared). Using IRt (first power of I) badly underestimates the dependence on current, the tempting linear form.
  19. In resistance spot welding with I = 200 A, interface resistance R = 0.02 Ω and weld time t = 0.1 s, the heat generated by H = I²Rt, in J, is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 80

    H = I²Rt = 200² × 0.02 × 0.1 = 40 000 × 0.002 = 80 J. Using IRt (200 × 0.02 × 0.1 = 0.4) drops one factor of I and grossly underestimates.
  20. A composite has 70% matrix (E = 3 GPa) and 30% fibre (E = 70 GPa) by volume, loaded transverse to the fibres. By the inverse rule of mixtures 1/E = Σ(V/E), the transverse modulus, in GPa (two decimals), is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 4.21

    1/E = 0.7/3 + 0.3/70 = 0.2333 + 0.0043 = 0.2376, so E = 4.21 GPa, dominated by the soft matrix. The direct rule (0.7×3 + 0.3×70 = 23.1) hugely overstates the transverse modulus.
  21. Hot isostatic pressing (HIP) of a powder part is used mainly to

    1. coat the part with polymer
    2. cut the part to shape
    3. eliminate residual porosity by applying heat and high gas pressure from all sides
    4. add porosity deliberately
    Show answer

    Answer: C — eliminate residual porosity by applying heat and high gas pressure from all sides

    HIP applies isostatic gas pressure at high temperature to close internal pores and reach near-full density. Adding porosity is the opposite of its purpose, the tempting reversal.