Ironmaking and Steelmaking in Numbers: Blast Furnace Thermodynamics and Material Balance, Heats of Reaction, Decarburisation and Desulphurisation Kinetics, Newton–Raphson and Probability

Section 4 of the Metallurgical Engineering paper names the thermodynamics of blast furnace ironmaking, associated heat effects, ladle processes and the kinetics of steelmaking, and Section 1 names non-linear equations of a single variable and the definitions of probability; the earlier chapters of both sections state them in words. The Boudouard reaction C + CO₂ = 2CO becomes favourable above 977 K; to make a tonne of hot metal at 94.5% Fe from a 60% Fe ore takes about 1591 kg of ore; burning carbon to CO releases 9.2 MJ/kg but to CO₂ 32.8 MJ/kg; a basic-oxygen converter blowing 41.5 kg of carbon per tonne to CO needs 38.7 Nm³ of oxygen; carbon in the second blowing regime falls from 0.7 to 0.05% in 10.6 min at k = 0.25 min⁻¹; and Newton–Raphson finds the root of x³ − 2x − 5 = 0 as 2.0946 in four steps.
Overview

Blast Furnace Ironmaking: Reduction Equilibria and the Material Balance

2 min read

In the stack, CO reduces the oxides stepwise (Fe₂O₃ → Fe₃O₄ → FeO → Fe) by the indirect reaction FeO + CO = Fe + CO₂ (slightly exothermic, below about 1000 K); in the hot lower part the coke carbon reduces FeO directly, FeO + C = Fe + CO (strongly endothermic). The two are tied by the Boudouard (solution-loss) reaction C + CO₂ = 2CO, ΔH ≈ +172.5 kJ and ΔS ≈ +176.5 J/K, so ΔG = ΔH − TΔS is zero at T = ΔH/ΔS = 977 K (about 704 °C): below that the gas is mainly CO₂, above it mainly CO. At 1 atm, the equilibrium CO fraction is 60% at 973 K and 99.3% at 1273 K — the reason the lower furnace is highly reducing. For FeO + C = Fe + CO with ΔH ≈ +154 kJ and ΔS ≈ +153 J/K, direct reduction becomes feasible above ΔH/ΔS = 1007 K at 1 atm. Material balance for 1 tonne of hot metal (94.5% Fe = 945 kg): from an ore with 60% Fe, with 99% of the iron recovered, ore = 945/(0.60 × 0.99) = 1591 kg; oxygen to be removed from Fe₂O₃ = 945 × 48/(2 × 55.85) = 406 kg; and if reduction were entirely by CO (3CO + Fe₂O₃ → 2Fe + 3CO₂) it would consume 1.5 mol CO per mol Fe, i.e. 711 kg of CO. In practice the gas also meets the thermal requirement, so the carbon rate is set by the heat more than by the chemistry (the Rist diagram combines the two on one operating line).

ReactionΔH, ΔS (approx.)Feasible above
C + CO₂ = 2CO+172.5 kJ, +176.5 J/K977 K
FeO + C = Fe + CO+154 kJ, +153 J/K1007 K
FeO + CO = Fe + CO₂Slightly exothermicFavoured at lower temperature

In the stack, CO reduces the oxides stepwise (Fe₂O₃ → Fe₃O₄ → FeO → Fe) by the indirect reaction FeO + CO = Fe + CO₂ (slightly exothermic, below about 1000 K); in the hot lower part the…

Associated Heat: Heats of Combustion and the Converter Heat Balance

1 min read

The heat released depends on the product: C + ½O₂ → CO releases 110.5 kJ/mol = 9.2 MJ/kg C, but C + O₂ → CO₂ releases 393.5 kJ/mol = 32.8 MJ/kg C — burning to CO₂ gives 3.6 times as much, so afterburning (CO to CO₂ above the bath) recovers a great deal of heat. In a basic-oxygen converter no external fuel is used: the heat comes from oxidising the impurities of 1 tonne of hot metal. Taking Si 8 kg to SiO₂ (ΔH = −910.7 kJ/mol: 32.4 MJ/kg), C 41.5 kg to CO (9.2), Mn 4 kg to MnO (−385 kJ/mol: 7.0 MJ/kg) and 20 kg of Fe to FeO (−272 kJ/mol: 4.9 MJ/kg) the heat generated is 259 + 382 + 28 + 97 = 767 MJ. Heating 1000 kg of metal from 1300 °C to 1650 °C at 0.8 kJ/kg·K needs 280 MJ; with, say, 150 MJ lost in slag, gas and radiation, the surplus can melt scrap that needs about 1.41 MJ/kg (heating from 25 to 1650 °C plus the latent heat): 239 kg — a scrap charge of about 20%, as in practice. Silicon is the strongest heat source per unit mass, which is why high-silicon hot metal allows more scrap but makes more slag. (The numbers are an illustrative balance, not a plant record.)

Heat source (per tonne hot metal)QuantityHeat (MJ)
Si → SiO₂8 kg259
C → CO41.5 kg382
Mn → MnO4 kg28
Fe → FeO20 kg97
Total—767

The heat released depends on the product: C + ½O₂ → CO releases 110.5 kJ/mol = 9.2 MJ/kg C, but C + O₂ → CO₂ releases 393.5 kJ/mol = 32.8 MJ/kg C — burning to CO₂ gives 3.6 times as much…

Kinetics of Steelmaking: Decarburisation and Desulphurisation

1 min read · 1 part

Oxygen demand: C + ½O₂ → CO consumes 0.5 × 22.4/12.01 = 0.933 Nm³ O₂ per kg C, so removing 41.5 kg of carbon from a tonne (4.2% to 0.05%) takes 38.7 Nm³ (the rest of the typical 55 Nm³/t goes to Si, Mn, P and Fe). Decarburisation has two regimes. At high carbon the rate is set by the oxygen supply and is constant (zeroth order in carbon, limited by the blowing rate); below a critical carbon (about 0.3–0.7%, depending on the blow) the rate is limited by mass transfer of carbon in the metal and is first order: −dC/dt = k (C − C), so C = C₀e^(−kt) with C ≈ 0. With k = 0.25 min⁻¹ the time to fall from 0.7% to 0.05% is t = ln(0.7/0.05)/k = 10.6 min, and each further factor of ten in carbon costs ln 10/0.25 = 9.2 min — which is why end-point control of low-carbon steel is slow, over-oxidises the bath (more FeO in slag, more dissolved oxygen) and needs deoxidation in the ladle with Al or Si–Mn. Desulphurisation is a slag–metal equilibrium: the sulphur partition L_S = (%S)slag/[%S]metal rises with basicity, low oxygen potential and temperature. With L_S = 50, 1000 kg of metal initially at 0.03% S (0.3 kg) and 100 kg of slag, the sulphur balance 0.3 = 10[%S] + 100 × 50[%S]/100 = 60[%S] gives [%S] = 0.005%: a basic reducing slag (CaO, low FeO) in the ladle removes it, whereas the oxidising BOF slag cannot.

ProcessRate lawNumber here
Oxygen for 41.5 kg C0.933 Nm³/kg38.7 Nm³
Decarburisation 0.7 → 0.05%ln(C₀/C)/k10.6 min
Desulphurisation, L_S = 50S balance0.005% S

Oxygen demand: C + ½O₂ → CO consumes 0.5 × 22.4/12.01 = 0.933 Nm³ O₂ per kg C, so removing 41.5 kg of carbon from a tonne (4.2% to 0.05%) takes 38.7 Nm³ (the rest of the typical 55 Nm³/t…

Newton–Raphson, Probability and Matrices for Metallurgists

2 min read · 2 parts

Newton–Raphson solves f(x) = 0 by the iteration x_(n+1) = x_n − f(x_n)/f′(x_n), converging quadratically near a simple root. For f(x) = x³ − 2x − 5 starting at x₀ = 2: x₁ = 2.1000, x₂ = 2.094568, x₃ = 2.094551, x₄ = 2.094551, the number of correct digits roughly doubling each step; a poor start near f′ = 0 can diverge, and the method is the standard way to invert non-linear thermodynamic relations such as K(T) for the equilibrium temperature. Probability: the classical definition counts equally likely outcomes, P = favourable/total; the relative-frequency definition is the limit of n_A/n; the axiomatic definition requires P(A) ≥ 0, P(S) = 1 and additivity for disjoint events. Among 20 castings, 3 are defective and 2 are drawn without replacement: P(both good) = C(17, 2)/C(20, 2) = 136/190 = 0.7158, so P(at least one defective) = 0.2842. Matrices: the 2 × 2 matrix [[4, 1], [2, 3]] has characteristic equation λ² − 7λ + 10 = 0, eigenvalues 5 and 2 (trace 7, determinant 10), and determinant 10 ≠ 0 so it is invertible — the type of calculation behind mass-balance systems and the diffusion matrices of multicomponent alloys.

nNewton iterate x_n for x³ − 2x − 5Error
02.000000009.5e-02
12.100000005.4e-03
22.094568121.7e-05
32.094551481.6e-10
42.094551480.0e+00
🎯 Blast-furnace stoichiometry, worked
The overall reduction Fe₂O₃ + 3CO → 2Fe + 3CO₂ gives 2 × 55.85 = 111.7 kg of iron per 159.7 kg of haematite, so 1000 kg of ore with 80% Fe₂O₃ yields 800 × 111.7/159.7 = 560 kg of iron. The carbon needed follows from the CO consumed: 3 mol CO per 2 mol Fe, that is 36/111.7 = 0.32 kg of carbon per kg of iron as CO alone, and in practice the coke rate is about 450 to 500 kg per tonne of hot metal because carbon also heats the furnace and carburises the metal.

Newton–Raphson solves f(x) = 0 by the iteration x_(n+1) = x_n − f(x_n)/f′(x_n), converging quadratically near a simple root. For f(x) = x³ − 2x − 5 starting at x₀ = 2: x₁ = 2.1000, x₂ =…

Key takeaways

  • The Boudouard reaction C + CO₂ = 2CO is feasible above ΔH/ΔS ≈ 977 K; direct reduction FeO + C becomes feasible near 1000 K; ore per tonne of hot metal = Fe in metal/(ore grade × recovery).
  • Burning C to CO releases 9.2 MJ/kg, to CO₂ 32.8 MJ/kg; the converter is autogenous from Si, C, Mn and Fe oxidation, and the surplus heat melts scrap.
  • Decarburisation is oxygen-supply controlled at high carbon (constant rate) and mass-transfer controlled below the critical carbon (first order, t = ln(C₀/C)/k).
  • Desulphurisation needs a basic, reducing slag: L_S = (%S)/[%S]; the oxidising BOF slag cannot do it.
  • Newton–Raphson x_(n+1) = x_n − f/f′ converges quadratically; classical probability = favourable/total; eigenvalues sum to the trace and multiply to the determinant.

Practice questions (24)

Attempt each one before opening the answer. Every explanation names the tempting wrong option as well as the right one, because that is where marks are lost.

  1. Using ΔH = +172.5 kJ and ΔS = +176.5 J/K for C + CO₂ = 2CO, the temperature in kelvin above which the reaction is spontaneous at standard conditions (nearest integer) is:

    Numerical answer — type the value.

    Show answer

    Answer: 977

    ΔG = ΔH − TΔS = 0 at T = 172 500/176.5 = 977 K. The reaction is endothermic with a gas-volume increase, so it is favoured at high temperature.
  2. A hot metal of 94.5% Fe is made from an ore of 60% Fe with 99% iron recovery. The mass of ore in kg per tonne of hot metal (nearest integer) is:

    Numerical answer — type the value.

    Show answer

    Answer: 1591

    945/(0.60 × 0.99) = 1591 kg. Ignoring the recovery gives 1575 kg.
  3. Why does burning coke to CO₂ at the tuyeres matter less to the heat supply than the later reaction C + CO₂ → 2CO suggests?

    1. CO₂ is a solid at those temperatures
    2. Coke does not burn at the tuyeres
    3. At the tuyere flame temperature carbon burns essentially to CO, releasing 9.2 MJ/kg, and CO₂ is converted back by the solution-loss reaction
    4. The reaction is exothermic
    Show answer

    Answer: C — At the tuyere flame temperature carbon burns essentially to CO, releasing 9.2 MJ/kg, and CO₂ is converted back by the solution-loss reaction

    The Boudouard equilibrium sits almost entirely on the CO side above about 1300 K, so carbon leaves the combustion zone as CO (110.5 kJ/mol); the remaining combustion heat to CO₂ is recovered only higher up. The solution-loss reaction itself is endothermic (+172.5 kJ).
Show the other 21 questions
  1. The heat released by burning 1 kg of carbon completely to CO₂ (ΔH = −393.5 kJ/mol, M = 12.011) in MJ (one decimal) is:

    Numerical answer — type the value.

    Show answer

    Answer: 32.8

    393.5/12.011 = 32.8 MJ/kg. Burning only to CO gives 9.2 MJ/kg, 28% of that.
  2. Below the critical carbon content, decarburisation is first order with k = 0.25 min⁻¹. The time to reduce carbon from 0.70% to 0.05% in minutes (one decimal) is:

    Numerical answer — type the value.

    Show answer

    Answer: 10.6

    t = ln(0.70/0.05)/0.25 = ln 14/0.25 = 10.6 min. Treating the rate as constant would give a wrong, linear estimate.
  3. Sulphur partition L_S = 50 between slag and metal; 1000 kg of metal starts at 0.03% S and is treated with 100 kg of slag. The final sulphur in the metal in per cent (three decimals) is:

    Numerical answer — type the value.

    Show answer

    Answer: 0.005

    Sulphur balance: 0.3 kg = 1000[%S]/100 + 100 × 50[%S]/100 = 10[%S] + 50[%S] = 60[%S], so [%S] = 0.005%. A bigger slag mass or higher L_S lowers it further.
  4. Newton–Raphson for f(x) = x³ − 2x − 5 starting at x₀ = 2 gives x₁ equal to:

    1. 3.0
    2. 1.5
    3. 2.5
    4. 2.1
    Show answer

    Answer: D — 2.1

    f(2) = −1 and f′(2) = 10, so x₁ = 2 − (−1)/10 = 2.1; the iteration then settles on the root 2.0946. A sign error in f(2) gives 1.9.
  5. Of 20 castings, 3 are defective. Two are drawn at random without replacement. The probability that both are good (four decimals) is:

    Numerical answer — type the value.

    Show answer

    Answer: 0.7158

    C(17, 2)/C(20, 2) = 136/190 = 0.7158. Multiplying 0.85 × 0.85 = 0.7225 would wrongly assume replacement.
  6. For the matrix [[4, 1], [2, 3]], which statements are correct?

    1. The matrix is singular
    2. The eigenvalues are 5 and 2
    3. The trace equals the sum of the eigenvalues
    4. The determinant is 10
    Show answer

    Answer: B — The eigenvalues are 5 and 2; C — The trace equals the sum of the eigenvalues; D — The determinant is 10

    λ² − 7λ + 10 = (λ − 5)(λ − 2); trace 7 = 5 + 2, determinant 10 = 5 × 2. A non-zero determinant means the matrix is invertible, not singular.
  7. In the blast furnace, the region where the iron-bearing burden softens and melts, forming semi-fused layers of low permeability between coke layers, is the:

    1. raceway
    2. hearth
    3. cohesive zone
    4. granular (lumpy) zone
    Show answer

    Answer: C — cohesive zone

    Between the lumpy zone above and the dripping zone below lies the cohesive zone, whose shape strongly controls gas distribution. The raceway is the tempting answer because it is also a hot, critical region, but it is the cavity in front of the tuyeres where coke burns in the blast.
  8. The sensible heat, in MJ, needed to raise 1000 kg of a material with mean specific heat 0.8 kJ/(kg·K) by 100 K is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 80

    Q = mcΔT = 1000 × 0.8 × 100 = 80 000 kJ = 80 MJ. Answering 80 000 gives the value in kJ without converting to MJ.
  9. A first-order reaction has a rate constant of 0.1 min⁻¹. Its half-life, in minutes, is ____ (to two decimal places).

    Numerical answer — type the value.

    Show answer

    Answer: 6.93

    t½ = ln 2/k = 0.693/0.1 = 6.93 min; check e^(−0.1 × 6.93) = 0.5. Answering 5 uses 1/(2k), which is not the half-life of a first-order process.
  10. Using the trapezoidal rule with step h = 0.5, the estimate of ∫₀¹ x² dx is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 0.375

    T = (h/2)[f(0) + 2f(0.5) + f(1)] = 0.25 × (0 + 0.5 + 1) = 0.375 (the exact value is 1/3, so the rule overestimates a convex function). Answering 0.333 gives the exact integral, not the trapezoidal estimate asked for.
  11. For a reaction obeying the Arrhenius equation k = A exp(−E/RT), a plot of ln k against 1/T is a straight line whose slope equals:

    1. E/R
    2. ln A
    3. −E/(RT)
    4. −E/R
    Show answer

    Answer: D — −E/R

    ln k = ln A − (E/R)(1/T), so the slope is −E/R and the intercept is ln A. ln A is the tempting answer because it also appears in the linear form, but it is the intercept; +E/R would give a rate falling with temperature.
  12. A reaction has an activation energy of 100 kJ/mol. By what factor does its rate constant increase when the temperature rises from 1000 K to 1100 K? (R = 8.314 J/mol·K; give two decimal places)

    Numerical answer — type the value.

    Show answer

    Answer: 2.98

    k₂/k₁ = exp[(E/R)(1/T₁ − 1/T₂)] = exp[12 028 × 9.09 × 10⁻⁵] = exp(1.093) = 2.98. Answering 1.10 assumes the rate scales with T itself, ignoring the exponential temperature dependence.
  13. Taking a mean specific heat of 0.75 kJ/(kg·K) for solid iron and a latent heat of fusion of 270 kJ/kg, the heat needed to take 1 kg of iron from 25 °C to fully molten at its melting point of 1538 °C, in kJ, is ____ (to the nearest kJ).

    Numerical answer — type the value.

    Show answer

    Answer: 1405

    Q = 0.75 × (1538 − 25) + 270 = 1 134.75 + 270 = 1 404.75 ≈ 1 405 kJ. Answering 1 135 stops at the sensible heat and forgets the latent heat needed to melt at constant temperature.
  14. Which change, by itself, raises the adiabatic flame temperature in the blast-furnace raceway?

    1. enriching the blast with oxygen
    2. injecting more pulverised coal
    3. adding steam (moisture) to the blast
    4. lowering the hot-blast temperature
    Show answer

    Answer: A — enriching the blast with oxygen

    Oxygen enrichment reduces the nitrogen that must be heated per unit of carbon burnt, raising flame temperature. Coal injection is the tempting answer because coal is a fuel, but its volatile matter cracks endothermically, so injection lowers flame temperature and is often paired with oxygen enrichment to compensate; steam is decomposed endothermically too.
  15. Using Simpson's 1/3 rule with step h = 1, the estimate of ∫₀² x³ dx is ____.

    Numerical answer — type the value.

    Show answer

    Answer: 4

    S = (h/3)[f(0) + 4f(1) + f(2)] = (1/3)(0 + 4 + 8) = 4, which equals the exact value x⁴/4 = 4 because Simpson's rule is exact for cubics. Answering 5 comes from the trapezoidal rule, (1/2)(0 + 2 + 8).
  16. In the shrinking-core model for a dense spherical particle, when the chemical reaction at the core surface is rate-controlling, the fractional conversion X varies with time t as:

    1. 1 − (1 − X)^(1/3) = t/τ
    2. 1 − 3(1 − X)^(2/3) + 2(1 − X) = t/τ
    3. X = t/τ
    4. ln(1 − X) = −t/τ
    Show answer

    Answer: A — 1 − (1 − X)^(1/3) = t/τ

    Under chemical control the core radius shrinks linearly with time, and r_c/R = (1 − X)^(1/3) gives 1 − (1 − X)^(1/3) = t/τ. The expression 1 − 3(1 − X)^(2/3) + 2(1 − X) is the tempting answer because it is the other standard result, but it applies when diffusion through the product (ash) layer controls.
  17. Each casting from a line is independently defective with probability 0.1. The probability that at least one of three castings is defective is ____ (to three decimal places).

    Numerical answer — type the value.

    Show answer

    Answer: 0.271

    P = 1 − 0.9³ = 1 − 0.729 = 0.271, the same as summing the binomial terms for 1, 2 and 3 defects. Answering 0.3 simply adds 0.1 three times, which double-counts cases with more than one defect.
  18. Dense spherical ore particles react under chemical-reaction control, with complete conversion taking τ = 60 min. The time, in minutes, to reach 90% conversion is ____ (to one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 32.2

    t = τ[1 − (1 − X)^(1/3)] = 60 × (1 − 0.1^(1/3)) = 60 × (1 − 0.4642) = 32.2 min. Answering 54 assumes conversion linear in time (X = t/τ), which ignores the shrinking reaction surface.
  19. During refining, 1.0 t of silicon dissolved in hot metal is oxidised to SiO₂ (ΔH = −910.9 kJ per mol SiO₂; Si = 28.09). The heat released, in GJ, is ____ (to one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 32.4

    1 t Si = 10⁶/28.09 = 35 600 mol; heat = 35 600 × 910.9 kJ = 3.24 × 10⁷ kJ = 32.4 GJ. Answering 0.9 treats the heat per mole as if it were per kilogram of silicon.
  20. A reaction's rate constant is 0.01 s⁻¹ at 1000 K and 0.04 s⁻¹ at 1100 K. Its activation energy, in kJ/mol, is ____ (R = 8.314 J/mol·K; nearest whole number).

    Numerical answer — type the value.

    Show answer

    Answer: 127

    E = R ln(k₂/k₁)/(1/T₁ − 1/T₂) = 8.314 × 1.386/(9.09 × 10⁻⁵) = 126.8 kJ/mol ≈ 127; substituting back reproduces the factor of 4. Using log₁₀ instead of ln gives about 55 kJ/mol, a common slip.
  21. Which of the following statements about the iron blast furnace are correct?

    1. The thermal reserve zone is a region in the shaft where gas and solid temperatures are nearly equal
    2. Indirect reduction of iron oxides by CO occurs mainly in the stack at lower temperatures
    3. Direct reduction, FeO + C → Fe + CO, is strongly endothermic and occurs at high temperature
    4. Raising the hot-blast temperature increases the coke rate
    Show answer

    Answer: A — The thermal reserve zone is a region in the shaft where gas and solid temperatures are nearly equal; B — Indirect reduction of iron oxides by CO occurs mainly in the stack at lower temperatures; C — Direct reduction, FeO + C → Fe + CO, is strongly endothermic and occurs at high temperature

    CO reduces hematite and magnetite to wüstite and iron in the stack; direct reduction consumes carbon and heat lower down; the thermal reserve zone (around 900-1000 °C) has nearly equal gas and solid temperatures. The hot-blast statement is the trap: more sensible heat brought in by the blast lowers, not raises, the coke needed per tonne of hot metal.