Phase Diagrams and the Lever Rule, True Stress–Strain, Polymers, Composites and Ceramics, Powder Metallurgy and Non-Destructive Testing

Section 4 of the Mechanical paper names several items of Materials and Manufacturing that the earlier chapters mention but do not teach: phase diagrams, engineering and true stress–strain diagrams, polymers, composites and ceramics, the fundamentals of powder metallurgy, and non-destructive testing methods. The first materials chapter taught crystal structure and heat treatment and put the iron–carbon diagram to work through the casting and forming chapters; this one supplies the missing tools. A phase diagram is a map of which phases are stable at each temperature and composition, and the lever rule reads the amounts off it. The true stress–strain curve removes the illusion that a metal weakens after the ultimate strength — it is the necking geometry, not the material, that falls. Polymers, composites and ceramics complete the four material families, each with one governing idea (chain mobility and glass transition; load shared between fibre and matrix; strong bonds without slip). Powder metallurgy shapes metal without melting, and NDT inspects without destroying; each method matches a defect type to a physical principle. Computed here: a 0.4 wt% C steel just below the eutectoid temperature is 51.2% pearlite and 48.8% proeutectoid ferrite; a carbon-fibre/epoxy ply with 60% fibre has a longitudinal modulus of 139.4 GPa but only 8.55 GPa transverse; and a 20 µs round-trip ultrasonic echo in steel reads a thickness of 59 mm.
Overview

Phase Diagrams, the Gibbs Phase Rule and the Lever Rule

2 min read · 1 part

A phase is a physically distinct, homogeneous portion of a system; an equilibrium phase diagram plots the stable phases against temperature and composition at fixed pressure. The Gibbs phase rule, at constant pressure, is F = C − P + 1 (C components, P phases, F degrees of freedom): in a single-phase region of a binary alloy F = 2 (temperature and composition may both change), in a two-phase region F = 1, and at an invariant point — eutectic (liquid → α + β), eutectoid (γ → α + β), peritectic (liquid + α → β) — three phases coexist and F = 0, so temperature and compositions are fixed. A horizontal line at an invariant temperature is the signature. In a two-phase region the tie line gives the compositions of the two phases at its ends, and the lever rule gives their amounts: with overall composition C₀ and end compositions C_α and C_β, W_α = (C_β − C₀)/(C_β − C_α) and W_β = (C₀ − C_α)/(C_β − C_α) — the fraction of a phase is the opposite arm over the whole tie line. Solidification of a binary alloy follows the same diagram: the liquidus is where freezing starts, the solidus where it ends, and a solid solution cores as the cooling is too fast for diffusion.

Iron–iron carbide. Key points: eutectoid at 0.76 wt% C and 727 °C (austenite → ferrite + cementite, the lamellar mixture pearlite); eutectic at 4.3 wt% C and 1147 °C (liquid → austenite + cementite, ledeburite); maximum solubility of carbon in ferrite 0.022% and in austenite 2.14%; cementite Fe₃C at 6.67%. Steels have under 2.14% C, cast irons above. Hypoeutectoid steels (< 0.76% C) cool to proeutectoid ferrite plus pearlite; hypereutectoid (> 0.76%) to proeutectoid cementite plus pearlite. Just below 727 °C, a 0.4 wt% C steel has proeutectoid ferrite fraction (0.76 − 0.4)/(0.76 − 0.022) = 0.4878 and pearlite 0.5122; the total cementite is (0.4 − 0.022)/(6.67 − 0.022) = 0.0569, of which only 11.1% of the pearlite is cementite. A 1.2 wt% C steel has proeutectoid cementite (1.2 − 0.76)/(6.67 − 0.76) = 0.0745 and pearlite 0.9255. More carbon means more pearlite, more strength and hardness, less ductility.

A phase is a physically distinct, homogeneous portion of a system; an equilibrium phase diagram plots the stable phases against temperature and composition at fixed pressure. The Gibbs…

Engineering and True Stress–Strain

2 min read · 2 parts

Engineering stress σ_e = F/A₀ and strain ε_e = ΔL/L₀ use the original dimensions; true stress σ_t = F/A (instantaneous area) and true strain ε_t = ∫dL/L = ln(L/L₀). While deformation is uniform (volume constant, A L = A₀ L₀) the conversions are σ_t = σ_e (1 + ε_e) and ε_t = ln(1 + ε_e). At σ_e = 400 MPa and ε_e = 0.2: σ_t = 400 × 1.2 = 480 MPa and ε_t = ln 1.2 = 0.1823. After necking begins these formulas no longer apply (the strain is localised); true stress must be computed from the measured neck area. The engineering curve peaks at the ultimate tensile strength and then falls because the area shrinks faster than the metal hardens; the true curve keeps rising to fracture, so the metal never weakens. Necking starts when dσ_t/dε_t = σ_t (the hardening rate can no longer keep up with the area loss), the point of maximum load. True strains are additive — two successive 10% engineering strains give ln 1.1 + ln 1.1 = ln 1.21 whereas the engineering strains compound to 21% — and symmetric: stretching to twice the length and compressing to half give +ln 2 and −ln 2.

Strain-hardening. In the plastic range most metals follow the Hollomon relation σ_t = K ε_tⁿ, with strength coefficient K and strain-hardening exponent n (0 for a perfectly plastic solid, about 0.1–0.5 for metals; high n means a metal that hardens quickly and draws well). From two points, (0.05, 300 MPa) and (0.2, 420 MPa): n = ln(420/300)/ln(0.2/0.05) = 0.2427 and K = 300/0.05^0.243 = 621 MPa. Necking at maximum load occurs when ε_t = n: for this metal at true strain 0.243, an engineering strain of e^n − 1 = 0.275 — a larger n postpones necking and improves the uniform elongation, which is why n is the property that sets the formability of sheet. Toughness is the area under the engineering curve (energy to fracture), resilience the area up to yield; hardness (Brinell, Vickers, Rockwell) correlates with UTS (for steels UTS ≈ 3.45 × HB MPa as a rule of thumb) and impact strength (Charpy, Izod) measures energy to break a notched bar, falling sharply at a ductile-to-brittle transition temperature in BCC metals but not in FCC.

Engineering stress σ_e = F/A₀ and strain ε_e = ΔL/L₀ use the original dimensions; true stress σ_t = F/A (instantaneous area) and true strain ε_t = ∫dL/L = ln(L/L₀). While deformation is…

Polymers, Composites and Ceramics

2 min read · 3 parts

Polymers are long-chain molecules. Thermoplastics (polyethylene, PVC, nylon, polystyrene) soften on heating and can be re-melted and moulded repeatedly; thermosets (epoxy, phenolics, polyester resins) cross-link irreversibly on curing and char instead of melting; elastomers (rubbers) are lightly cross-linked chains that stretch several hundred per cent and recover. The glass-transition temperature T_g is where an amorphous polymer changes from a hard glassy to a soft rubbery state as chain segments become mobile; the melting temperature T_m applies to the crystalline fraction of semi-crystalline polymers. Below T_g the polymer is stiff and brittle; between T_g and T_m a thermoplastic is leathery and forms best. Strength and stiffness rise with crystallinity, chain length (degree of polymerisation) and cross-linking; behaviour is viscoelastic (creep, stress relaxation) and strongly temperature- and rate-dependent. Typical forming: injection moulding, extrusion, blow moulding, thermoforming for thermoplastics; compression and transfer moulding for thermosets.

Composites combine a reinforcement (fibres of glass, carbon or aramid; particles) with a matrix (polymer, metal, ceramic) so that the pair outperforms either. The matrix holds and protects the fibres and transfers load; the fibres carry it. For continuous aligned fibres, with fibre volume fraction V_f: loaded along the fibres (isostrain, Voigt) E_∥ = V_f E_f + (1 − V_f) E_m; loaded across (isostress, Reuss) 1/E_⊥ = V_f/E_f + (1 − V_f)/E_m. For carbon fibre (E_f = 230 GPa) in epoxy (E_m = 3.5 GPa) with V_f = 0.6: E_∥ = 139.4 GPa (the fibres carry 99% of the load) and E_⊥ = 8.55 GPa — roughly sixteen times weaker across, which is why plies are laid at several angles. Ceramics (alumina, silicon carbide, zirconia, glass) have ionic–covalent bonds that resist dislocation motion: very high hardness, melting point and compressive strength, low density and good wear and chemical resistance, but no ductility, low fracture toughness and a strength governed by the largest flaw (hence Weibull statistics, and compressive strength roughly ten times the tensile). They are shaped by powder processing and sintering, and cermets (WC–Co cutting tips) mix ceramic hardness with a metal binder's toughness.

FamilyStrengthTypical weakness
Metals and alloysgood, ductilecorrosion, density, fatigue
Polymerslow, but light and mouldablelow T_g, creep, ageing
Ceramicshigh compressive, hardbrittle; flaw-controlled
Compositesvery high specific strength along fibresanisotropy, delamination, cost
Three kinds of polymer
Polymers
  • ThermoplasticsSoften on heating; re-meltable
  • ThermosetsCross-link irreversibly; char
  • ElastomersLightly cross-linked; stretch and recover

Polymers are long-chain molecules. Thermoplastics (polyethylene, PVC, nylon, polystyrene) soften on heating and can be re-melted and moulded repeatedly; thermosets (epoxy, phenolics…

Powder Metallurgy and Non-Destructive Testing

3 min read · 4 parts

Powder metallurgy (P/M) forms parts from metal powder without melting. Steps: (1) powder production — atomisation (a molten stream broken by gas or water jets; the commonest, giving spherical powder), chemical reduction of oxides, electrolytic deposition, milling; (2) blending with lubricant and alloying powders; (3) compaction in a die at pressures of a few hundred MPa to a green compact of about 80–90% density — strong enough to handle, not to use, with density varying with the die friction (hence double-acting punches); (4) sintering below the melting point (typically 70–90% of T_m in K) in a protective atmosphere, where atoms diffuse across particle contacts and the compact bonds and shrinks; (5) sizing, impregnation, infiltration or heat treatment as needed. Typical products: self-lubricating porous bearings (oil impregnated in the pores), filters, gears and structural parts in high volume at low cost, cemented carbide tools (WC powder with cobalt binder, liquid-phase sintered), refractory metals such as tungsten that cannot be cast, and magnets and friction materials. Limits: part size and complexity (powder does not flow sideways), residual porosity (lower strength and fatigue), and powder cost. A 6.6 g/cm³ green iron compact is 84% of the 7.87 g/cm³ solid density.

Non-destructive testing finds defects without damaging the part; each method suits a defect type. Visual inspection; liquid penetrant (dye drawn into surface-breaking cracks by capillarity, any non-porous material); magnetic particle (flux leakage at surface and near-surface cracks collects iron powder; ferromagnetic materials only); eddy current (impedance change of a coil near a conductor, sensitive to surface cracks, conductivity and coating thickness; conductors only); ultrasonic (pulse-echo of 0.5–10 MHz waves; finds internal planar flaws and measures thickness; needs a couplant); radiography (X- or γ-ray absorption on film or detector; finds volumetric defects — porosity, inclusions — and is poor for cracks lying perpendicular to the beam; radiation hazard); and acoustic emission (listens for the stress waves of growing cracks). In pulse-echo ultrasonics thickness t = v Δt/2 with v the wave speed: a round-trip time of 20 µs in steel at 5900 m/s gives t = 5900 × 20×10⁻⁶ / 2 = 59 mm. An echo falling from amplitude 0.8 to 0.2 has dropped 12.0 dB (20 log₁₀ ratio); a 6 dB drop is a factor 2.00 in amplitude.

MethodFindsLimitation
Liquid penetrantsurface-breaking cracks, laps, porositysurface only; non-porous materials
Magnetic particlesurface and near-surface cracksferromagnetic materials only
Eddy currentsurface cracks, conductivity, thicknessconductors only; shallow depth
Ultrasonicinternal planar defects, thicknessneeds couplant and skilled interpretation
Radiographyinternal volumetric defects (porosity, inclusions)poor for cracks normal to the beam; radiation hazard
🎯 A lever rule and a pearlite fraction
In a two-phase field the fraction of a phase is the opposite lever arm over the whole tie line. An alloy of 40% B lying between an α phase of 10% B and a β phase of 70% B has W_α = (70 − 40)/(70 − 10) = 0.5 and W_β = 0.5. In steel, the eutectoid is near 0.76% C and ferrite holds at most about 0.022% C, so a 0.4% C steel just below the eutectoid temperature is (0.4 − 0.022)/(0.76 − 0.022) = 0.51 pearlite, the rest proeutectoid ferrite. Austenite dissolves up to about 2.14% C, and cast iron begins above that, with the eutectic near 4.3% C.
Powder metallurgy, step by step
  1. Powder productionAtomisation is the commonest
  2. BlendingWith lubricant and alloying powders
  3. CompactionGreen compact, about 80–90% density
  4. SinteringBelow the melting point
  5. Finishing as neededSizing, impregnation, infiltration, heat treatment

Powder metallurgy (P/M) forms parts from metal powder without melting. Steps: (1) powder production — atomisation (a molten stream broken by gas or water jets; the commonest, giving…

Key takeaways

  • Phase rule at constant pressure F = C − P + 1; invariant points (eutectic, eutectoid, peritectic) have three phases and F = 0; lever rule: fraction of a phase = opposite arm / tie-line length.
  • Fe–Fe₃C: eutectoid 0.76% C at 727 °C (pearlite), eutectic 4.3% C at 1147 °C, ferrite 0.022%, austenite 2.14%, cementite 6.67%; steels below 2.14% C, cast irons above.
  • True stress σ_t = σ_e(1 + ε_e), true strain ε_t = ln(1 + ε_e) until necking; Hollomon σ = Kεⁿ; necking at maximum load when ε_t = n; the true curve never falls.
  • Composites: E_∥ = V_fE_f + (1 − V_f)E_m (isostrain), 1/E_⊥ = V_f/E_f + (1 − V_f)/E_m (isostress); thermoplastics re-melt, thermosets do not; ceramics are strong in compression and flaw-limited in tension.
  • Powder metallurgy: powder → blend → compact → sinter (below T_m, ~70–90% in K) → finish; good for porous bearings, carbides, refractory metals. NDT: penetrant (surface), magnetic particle (ferromagnetic), eddy current (conductors), ultrasonic (internal planar, t = vΔt/2), radiography (volumetric).

Practice questions (24)

Attempt each one before opening the answer. Every explanation names the tempting wrong option as well as the right one, because that is where marks are lost.

  1. In a two-phase region of a binary phase diagram, the weight fraction of phase α for overall composition C₀ and tie-line end compositions C_α and C_β is:

    1. (C₀ − C_α)/(C_β − C_α)
    2. C₀/C_α
    3. (C_β − C₀)/(C_β − C_α)
    4. (C_β − C_α)/(C_β − C₀)
    Show answer

    Answer: C — (C_β − C₀)/(C_β − C_α)

    Lever rule: the fraction of a phase is the length of the opposite arm of the lever over the whole tie line. The second option is the β fraction.
  2. At the eutectoid point of a binary system, the number of degrees of freedom at constant pressure is:

    1. 2
    2. 1
    3. 0
    4. 3
    Show answer

    Answer: C — 0

    Three phases coexist (γ, α, Fe₃C), so F = C − P + 1 = 2 − 3 + 1 = 0: temperature and all compositions are fixed, shown by the horizontal line at 727 °C.
  3. Just below 727 °C, a plain-carbon steel with 0.4 wt% C contains pearlite in a fraction nearest to (eutectoid 0.76 % C, ferrite 0.022 % C):

    1. 0.488
    2. 0.526
    3. 0.057
    4. 0.512
    Show answer

    Answer: D — 0.512

    Pearlite fraction = (0.4 − 0.022)/(0.76 − 0.022) = 0.512; the proeutectoid ferrite is the remaining 0.488. The 0.057 option is the total cementite fraction, a different quantity.
Show the other 21 questions
  1. A tensile test gives engineering stress 400 MPa at engineering strain 0.2, still before necking. The true stress and true strain are nearest to:

    1. 480 MPa and 0.182
    2. 480 MPa and 0.200
    3. 333 MPa and 0.182
    4. 400 MPa and 0.200
    Show answer

    Answer: A — 480 MPa and 0.182

    σ_t = σ_e(1 + ε_e) = 400 × 1.2 = 480 MPa and ε_t = ln 1.2 = 0.1823. True strain is always smaller than engineering strain for tension, and true stress larger.
  2. A metal has true stress 300 MPa at true strain 0.05 and 420 MPa at true strain 0.2 (σ = Kεⁿ). Find the strain-hardening exponent n to two decimals.

    Numerical answer — type the value.

    Show answer

    Answer: 0.24

    n = ln(420/300)/ln(0.2/0.05) = ln 1.4/ln 4 = 0.2427. Necking at maximum load then starts at true strain ε_t = n = 0.243.
  3. Which statement distinguishes a thermoset from a thermoplastic?

    1. A thermoset softens on every heating cycle
    2. A thermoset has a lower density always
    3. A thermoset has no covalent bonds
    4. A thermoset cross-links irreversibly on curing and cannot be re-melted
    Show answer

    Answer: D — A thermoset cross-links irreversibly on curing and cannot be re-melted

    Cross-linking in thermosets (epoxy, phenolics) locks the network in place so heating chars rather than melts them. Thermoplastics (PE, PVC, nylon) are linear or branched and soften reversibly.
  4. Carbon fibre (230 GPa) in epoxy (3.5 GPa), fibre volume fraction 0.6. The longitudinal modulus (isostrain) is nearest to:

    1. 8.6 GPa
    2. 139.4 GPa
    3. 233.5 GPa
    4. 116.8 GPa
    Show answer

    Answer: B — 139.4 GPa

    E_∥ = 0.6 × 230 + 0.4 × 3.5 = 139.4 GPa. The 8.6 GPa figure is the transverse (isostress) modulus, 1/E = 0.6/230 + 0.4/3.5.
  5. In powder metallurgy, sintering is carried out:

    1. below the melting point of the main constituent, so that atoms diffuse and bond particles
    2. above the melting point of all constituents
    3. at room temperature under high pressure only
    4. before compaction
    Show answer

    Answer: A — below the melting point of the main constituent, so that atoms diffuse and bond particles

    The green compact is heated below T_m (typically 70–90% of the absolute melting temperature) in a protective atmosphere; solid-state diffusion forms bonds between particles. It follows compaction, not precedes it.
  6. Which NDT method can detect only surface-breaking flaws and works on any non-porous material, magnetic or not?

    1. liquid penetrant testing
    2. radiography
    3. ultrasonic testing
    4. magnetic particle testing
    Show answer

    Answer: A — liquid penetrant testing

    Penetrant relies on capillary action into open cracks, so it finds only surface-breaking flaws, in any non-porous material. Magnetic particle needs a ferromagnetic part; ultrasonics and radiography reach the interior.
  7. A pulse-echo ultrasonic gauge in steel (wave speed 5900 m/s) records a round-trip time of 20 µs. The thickness is nearest to:

    1. 29.5 mm
    2. 5.9 mm
    3. 118 mm
    4. 59 mm
    Show answer

    Answer: D — 59 mm

    The pulse travels to the back wall and returns, so t = v Δt/2 = 5900 × 20×10⁻⁶/2 = 0.059 m = 59 mm. Forgetting the division by 2 gives 118 mm.
  8. In a two-phase α + β region of a binary diagram at some temperature, the α phase has 20 wt% B and the β phase has 60 wt% B. An alloy of 40 wt% B overall composition contains a weight fraction of α equal to _____ (one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 0.5

    Lever rule: W_α = (C_β − C₀)/(C_β − C_α) = (60 − 40)/(60 − 20) = 20/40 = 0.5. The lever arm for α is the one on the OPPOSITE side, from C₀ to C_β; the other arm, (40 − 20)/(60 − 20), is the β fraction, which happens to equal 0.5 here by symmetry.
  9. Gibbs' phase rule at constant pressure for a binary alloy (C = 2) is F = C − P + 1. In the two-phase region (P = 2) the number of degrees of freedom is:

    1. 3
    2. 2
    3. 0
    4. 1
    Show answer

    Answer: D — 1

    F = 2 − 2 + 1 = 1: one variable (the temperature) can be changed freely, and the compositions of the two phases are then fixed by the tie line. At an invariant point such as the eutectic (P = 3) F = 0, which is the tempting answer for any two-phase boundary.
  10. A tensile specimen carries an engineering stress of 300 MPa at an engineering strain of 0.1 (before necking). The true stress, in MPa, is _____.

    Numerical answer — type the value.

    Show answer

    Answer: 330

    σ_true = σ_eng(1 + e) = 300 × 1.1 = 330 MPa, because the cross-section shrinks as the length grows at constant volume. The true stress is always higher than the engineering stress in tension. Using ln(1.1) = 0.095 would give the true strain, not the stress.
  11. Which of the following is a thermoplastic polymer?

    1. Bakelite (phenol-formaldehyde)
    2. Epoxy resin
    3. Polyethylene
    4. Melamine-formaldehyde
    Show answer

    Answer: C — Polyethylene

    Polyethylene has linear or branched chains held by weak secondary bonds, so it softens on heating and can be re-melted and reshaped. Bakelite, cured epoxy and melamine-formaldehyde are cross-linked networks, thermosets that char instead of melting.
  12. A pulse-echo ultrasonic gauge in steel (wave speed 5900 m/s) records a round-trip time of 10 µs. The thickness, in mm, is _____ (one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 29.5

    The pulse travels the thickness twice, so t = v × time/2 = 5900 × 10 × 10⁻⁶/2 = 0.0295 m = 29.5 mm. Forgetting the factor 2 gives 59 mm.
  13. Magnetic particle inspection can be used to detect surface and near-surface flaws in:

    1. ferromagnetic materials such as carbon steel
    2. aluminium alloys
    3. any non-porous material, magnetic or not
    4. austenitic stainless steel only
    Show answer

    Answer: A — ferromagnetic materials such as carbon steel

    The method needs the part to be magnetised so that a flaw leaks flux and attracts the iron particles: it applies to ferromagnetic materials (iron, carbon steel, nickel). Aluminium and austenitic stainless steel are not ferromagnetic. Dye-penetrant testing is the one that works on any non-porous material.
  14. A plain-carbon steel with 0.6 wt% C is cooled slowly to just below 727 °C (eutectoid composition 0.77 wt% C, ferrite solubility 0.022 wt% C). The weight fraction of pearlite is, correct to three decimal places, _____.

    Numerical answer — type the value.

    Show answer

    Answer: 0.773

    Just below the eutectoid temperature the austenite of 0.77 wt% C becomes pearlite and the rest is proeutectoid ferrite. Lever rule: W_pearlite = (0.6 − 0.022)/(0.77 − 0.022) = 0.578/0.748 = 0.773. The simple ratio 0.6/0.77 = 0.78 ignores the 0.022 wt% C already in the ferrite.
  15. Carbon fibre (E = 230 GPa) in epoxy (E = 3.5 GPa) at a fibre volume fraction of 0.6 is loaded transversely (isostress model). The transverse modulus, in GPa, is _____ (two decimal places).

    Numerical answer — type the value.

    Show answer

    Answer: 8.55

    For loading across the fibres both constituents carry the same stress, so 1/E_T = V_f/E_f + V_m/E_m = 0.6/230 + 0.4/3.5 = 0.002609 + 0.114286 = 0.116895, giving E_T = 8.55 GPa. The rule of mixtures along the fibres would give 0.6 × 230 + 0.4 × 3.5 = 139.4 GPa, an isostrain result that does not apply across the fibres.
  16. A metal follows σ = Kεⁿ with K = 500 MPa and n = 0.2. The true stress at a true strain of 0.1, in MPa, is _____ (one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 315.5

    σ = 500 × 0.1^0.2 = 500 × 0.631 = 315.5 MPa. The value 100 would come from 500 × 0.1 × 2, treating the exponent as a multiplier, and 50 from dropping the exponent altogether.
  17. A metal obeys σ = Kεⁿ with n = 0.25. Necking begins when the true strain equals n (Considère's criterion). The corresponding engineering strain at the onset of necking, correct to three decimal places, is _____.

    Numerical answer — type the value.

    Show answer

    Answer: 0.284

    Necking starts at true strain ε = n = 0.25. The engineering strain follows from ε = ln(1 + e), so e = e0.25 − 1 = 1.2840 − 1 = 0.284. The value 0.25 treats the true and engineering strains as equal, which they are only for small strains.
  18. In the Pb–Sn system the eutectic composition is 61.9 wt% Sn and the maximum solubility of Sn in α is 19.2 wt% Sn. An alloy of 40 wt% Sn is cooled to just above the eutectic temperature (183 °C). The weight fraction of proeutectic α is, correct to three decimal places, _____.

    Numerical answer — type the value.

    Show answer

    Answer: 0.513

    Just above 183 °C the alloy consists of proeutectic α (19.2 wt% Sn) and liquid at the eutectic composition (61.9 wt% Sn). Lever rule: W_α = (61.9 − 40)/(61.9 − 19.2) = 21.9/42.7 = 0.513. The remaining 0.487 is the liquid that freezes into the eutectic mixture. The ratio (40 − 19.2)/(61.9 − 19.2) = 0.487 is the liquid fraction, the tempting wrong choice of lever arm.
  19. A sintered powder-metal compact of mass 100 g occupies a volume of 15 cm³. The theoretical (fully dense) density of the metal is 7.8 g/cm³. The porosity of the compact, in per cent, is _____ (one decimal place).

    Numerical answer — type the value.

    Show answer

    Answer: 14.5

    Compact density = 100/15 = 6.667 g/cm³. Relative density = 6.667/7.8 = 0.8547, so porosity = 1 − 0.8547 = 0.1453 = 14.5%. The relative density 85.5% is the tempting answer if the question is read as density rather than pore fraction.
  20. Which of the following statements comparing thermoplastics and thermosets are correct? (More than one option may be correct.)

    1. Thermoplastics soften on heating and can be remelted
    2. Thermosets have a cross-linked network structure
    3. Thermosets cannot be remelted once cured
    4. Thermosets are easier to recycle by remelting than thermoplastics
    Show answer

    Answer: A — Thermoplastics soften on heating and can be remelted; B — Thermosets have a cross-linked network structure; C — Thermosets cannot be remelted once cured

    Thermoplastics are held together by weak secondary bonds between chains, which loosen on heating, so they can be softened repeatedly. Thermosets form covalent cross-links on curing and degrade rather than melt, so they cannot be remelted. The last statement reverses the truth: remelting is exactly what thermoplastics allow.
  21. Which of the following statements about non-destructive testing methods are correct? (More than one option may be correct.)

    1. Magnetic particle inspection can be used on aluminium castings
    2. Radiography can reveal internal volumetric flaws such as porosity
    3. Eddy-current testing can detect surface and near-surface flaws in electrically conducting materials
    4. Dye-penetrant testing can reveal subsurface voids that do not reach the surface
    Show answer

    Answer: B — Radiography can reveal internal volumetric flaws such as porosity; C — Eddy-current testing can detect surface and near-surface flaws in electrically conducting materials

    Radiography uses penetrating radiation and shows internal voids and inclusions through density differences. Eddy-current testing works on any electrical conductor, to a limited depth. Magnetic particle inspection needs a ferromagnetic part, and aluminium is not. Dye penetrant needs the flaw to be open to the surface so that liquid can enter it, so closed subsurface voids stay invisible.